For sterile barrier systems such as paper/film pouches and lidded trays, seal strength is the quantitative measure of how robust a seal is and how consistently the sealing process produces it. US files often cite ASTM F88/F88M; the Chinese counterpart is YY/T 0681.2-2010. The same seal can give different numbers if you change the tail-holding technique or the specimen width. This article covers the test method itself, not the sealing process window. Clause numbers refer to ASTM F88/F88M-23.
The short answer
- Use one technique for a whole test series. Clause 4.2 notes that part of the measured force may be a bending component, that each technique affects results differently, and that one technique (A, B or C) should be used consistently throughout a test series. The report must state which one (clause 10.1.10).
- A is unsupported, B is supported at 90° by hand, C is supported at 180°. In the 2023 edition, Technique C also covers rigid and semi-rigid components such as trays.
- Three widths, one range of rates. Clause 6.2 gives specimen widths of 25 mm, 15 mm or 25.4 mm (1 in.); clause 9.7 sets grip separation at 200 mm/min to 300 mm/min.
- Always report maximum force; report average force only when the failure mode supports it. When the strip peels apart in the seal area, average peel force may be an important index; when separation is largely by breaking, tearing or elongation, it should not be reported (clauses 9.8 and 9.9).
- A CMA mark is only possible under YY/T 0681.2-2010. SUNGO Shanghai's CNAS schedule lists ASTM F88/F88M-23 and YY/T 0681.2-2010; its CMA schedule lists only YY/T 0681.2-2010; its IAS scope lists ASTM F88/F88M and YY/T 0681.2 without edition years. This test is not within the Hefei laboratory's CNAS, CMA or IAS scope.
- The method sets no pass/fail values. Clause 4.1 only says a minimum is needed and an upper limit is sometimes desirable; the values come from the product or packaging specification.
Standards and scope
Sources: the ASTM product page and the publicly available sample pages of the standard, the US FDA Recognized Consensus Standards database, and China's national standards information platform, checked on 22 October 2026.
ASTM F88/F88M-23
- Standard Test Method for Seal Strength of Flexible Barrier Materials, under ASTM Committee F02 on Primary Barrier Packaging and Subcommittee F02.20 on Physical Properties.
- Approved 1 May 2023 and published August 2023. Originally approved in 1968; the previous edition was F88/F88M-21.
- Scope: measures the strength of seals between a flexible material and another flexible, rigid or semi-rigid material, by the force needed to separate a test strip containing the seal, and identifies the failure mode. Separating a whole lid from a rigid or semi-rigid round container is covered by ASTM F2824.
- The FDA Recognized Consensus Standards database lists this edition as recognition number 14-596, entered 18 December 2023, complete standard. Recognition of a standard does not mean any particular report will be accepted.
YY/T 0681.2-2010
- Test methods for sterile medical device package, Part 2: Seal strength of flexible barrier materials. A recommended pharmaceutical industry standard, issued 27 December 2010, effective 1 June 2012, shown as current on the national platform.
- Since it was issued, ASTM has published F88 editions -15, -21 and -23. Check details such as techniques and specimen preparation against the text of YY/T 0681.2.
Differences between the -21 and -23 abstracts
- Clause 1.2: in the -21 abstract this clause mentions only seals between a flexible and a rigid material; -23 lists another flexible material, a rigid material or a semi-rigid material, adding semi-rigid counterparts explicitly. This does not mean -21 excluded flexible-to-flexible seals: the Technique C description in -21 is the one that -23 now assigns to flexible-to-flexible seals.
- Technique C: -21 gives one description (least flexible tail flat on a rigid alignment plate, the other folded back 180°). -23 limits that to flexible-to-flexible seals and adds that, for rigid and semi-rigid applications, the structure of the least flexible side may be kept and gripped or fixtured.
If earlier reports used -21 or older, check that technique and specimen preparation match before comparing data.
Techniques A, B and C
The unsealed material on each side of the seal is the tail. Each tail is clamped in opposing grips, which move apart at a constant rate until the seal fully separates. The techniques differ in whether and how the seal is supported, in order to control the bending component.
| Technique | What the standard says (clause 4.2) | Points to watch |
|---|---|---|
| A: Unsupported | Each tail is secured in opposing grips; the seal is unsupported. | Each technique affects the bending component differently (clause 4.2); compare only with data from the same technique. |
| B: Supported 90° (by hand) | Each tail is secured; the seal is held by hand at 90° to the tails. | Note 4: excessive lateral force affects results; contact should be loose, only stopping the tail moving up or down. |
| C: Supported 180° | Flexible to flexible: the least flexible tail is typically supported flat on a rigid alignment plate held in one grip; the more flexible tail is folded 180° over the seal into the other grip. Rigid or semi-rigid: the structure of the least flexible side may be kept and gripped or fixtured. | Note 5: tail movement or flipping should be reported. Appendix X4 shows optional fixtures. |
How to choose
- Existing requirements first. If a specification or earlier validation report names a technique, keep it. Comparisons before and after aging or sterilization, or between lots, need the same technique, width and rate.
- Then the materials. Paper/film and film/film pouches are flexible-to-flexible, and any technique may be used. Lids on trays are flexible-to-rigid or semi-rigid, which the 2023 version of Technique C specifically addresses.
- Cover it in test method validation. Note 6 says fixtures, alignment plates and which material goes in which grip are known to affect results and should be addressed in validation, with reference to ASTM F3263.
- Do not compare across techniques. Test Series 2 of the precision study (uncoated Tyvek sealed to PET/LDPE film) used 90° supported, unsupported, 180° supported and reversed-grip set-ups, and the grand averages for the same material differed between them.
Specimen width, separation rate and grip distance
- Width: clause 6.2 calls for a cutter conforming to 6.5 of ASTM D882, giving 25 mm (0.984 in.), 15 mm (0.591 in.) or 25.4 mm (1.00 in.) strips, so 25 mm and 25.4 mm are listed as separate options; clause 1.6 requires SI and inch-pound values to be used independently and not combined. Note 11: seal strength is proportional to width under the same conditions. Note 10: any deviation from the specified width needs a documented rationale or data.
- Cutting: clause 9.2 asks for the Fig. 2 dimensions, with clean edges perpendicular to the seal; several locations around the package may be tested.
- Rate: clause 6.1 requires a constant rate-of-jaw-separation tester recording load and grip separation; clause 9.7 sets 200 mm/min to 300 mm/min (8 in./min to 12 in./min). Appendix X3 discusses the effect of rate.
- Grip distance: clause 9.4 recommends, for seals between flexible materials, 10 mm for highly extensible and 25 mm for less extensible materials in fin and hot-wire seals, and X + 10 mm for lap seals (X is the seal dimension). For lids on trays it depends on tray size and design (Annexes A1 and A2).
- Conditioning and orientation: if conditioning before testing is needed, see ASTM E171 (clause 8.1). Fin-seal tail orientation can significantly affect results, and the report should describe how it was controlled (clause 9.6).
Maximum force or average force?
Clause 3.1 defines maximum seal strength as the maximum force per unit width to fully separate the seal, and average seal strength as the average force per unit width, normally calculated from the force versus grip travel plot. The initial ramp-up and the return to zero are excluded, and the same amount of data must be discarded for every test in a comparison.
- Report maximum force for every specimen and identify the failure mode (clause 9.8).
- If the strip peels apart in the seal area, by adhesive failure, cohesive failure or delamination, average peel force may be an important index (clause 9.9). Fig. 3 illustrates an algorithm using only the central 80 % of the curve; state the algorithm when average peel force is reported (clause 10.1.16).
- If separation is largely by breaking, tearing or elongation, average force should not be reported (clause 9.9.2); where it is withheld for individual specimens, record why (Note 14).
- Maximum force is preferably expressed in N/m or lbf/in. of original specimen width (clause 10.1.15), to three significant figures (clause 10.1.9). If a specification is written per width, such as N/15 mm, the report should state the matching specimen width.
Recording the failure mode
Clause 10.1.14 calls for a visual determination of failure mode; one strip often shows several, and all should be recorded. Fig. 4 suggests:
- Adhesive failure at the seal interface, that is, a peel.
- Cohesive failure within a material.
- The material breaks or tears in the seal area or at the seal edge.
- A surface layer delaminates from its substrate.
- The material elongates.
- The material breaks or tears away from the seal.
Under clause 9.9, adhesive failure, cohesive failure and delamination count as peeling apart in the seal area, so average peel force can be calculated; when the strip does not peel significantly and separation is by breaking, tearing or elongation, it is not reported. Clause 9.11 adds that energy-type measures apply only to pure peel and need caution when other modes occur.
Pouches and trays: reading curves and spotting anomalies
Clause 9.10 suggests plotting force against grip travel where it helps. For a specific product, the validation protocol and specification take precedence.
Paper/film pouches (flexible to flexible)
One side is a porous material such as medical paper or a nonwoven, the other is plastic film, and the seal is usually designed to peel open in use. The curve has an initial ramp-up that does not represent seal strength, a peel region where force fluctuates within a band and from which average peel force is taken, and a return to zero that is also excluded. Watch for:
- A layer lifted from the porous surface or fibers torn out: separation was not only at the seal interface. Record each mode against Fig. 4; peel and delamination may both be present.
- A break at the seal edge or away from the seal: maximum force reflects the material, not the seal. Report it with the mode, without average force.
- Record which material was in which grip (clause 10.1.11). For film/film pouches where the webs look alike, label each tail first (Note 12).
Trays and blisters (flexible to rigid or semi-rigid)
- Preparation (clause 9.3): where flange and seal geometry allow, cut through the lid only and leave the rigid part intact, or cut through the flange. Either is acceptable, but data to be compared must be prepared the same way. Avoid damaging the seal or injuring the operator.
- Holding: Technique C allows the tray structure to be kept and gripped or fixtured.
- Interferences (clause 5.1): elongation, flexing around the flange, flange shape and caliper variation can add components unrelated to seal strength (Annex A1). If the curve shows fluctuations that do not fit a peel, check these first and note them in the report (clause 10.1.13).
Quick reference
| What you see | Likely meaning | What to do (clause) |
|---|---|---|
| Force rises then drops sharply; the strip breaks at the seal edge or away from it | Material failed before the seal | Report maximum force and mode; no average force (9.8, 9.9.2) |
| The strip stretches and force keeps rising | Material elongation | Record the mode; limit grip distance for highly extensible materials; no average force (9.4 footnote, 9.9.2) |
| Wide scatter with Technique B | Inconsistent lateral hand force | Standardize handling or use a fixture; assess in method validation (Notes 4 and 6) |
| Large differences between locations on one package | Seal not uniform around the perimeter | Report by location and review the sealing process (9.2) |
A seal that meets its strength specification can still have a leak channel; strength and integrity are different tests.
ASTM F88 and YY/T 0681.2-2010 side by side
| Item | ASTM F88/F88M-23 | YY/T 0681.2-2010 |
|---|---|---|
| Type | ASTM standard test method | Recommended Chinese pharmaceutical industry standard |
| Dates | Approved 1 May 2023, published August 2023 | Issued 27 December 2010, effective 1 June 2012 |
| Techniques, width, rate | See above | Refer to the text of the standard |
| Marks at SUNGO Shanghai | CNAS (-23 edition); IAS (no edition year); not on the CMA schedule | CNAS and CMA (-2010 edition); IAS (no edition year) |
A report states only the standard actually used; if one lot needs both, list both in the order.
Accreditation scope table
Rows taken from the CNAS and CMA schedules and the IAS scope of Shanghai SUNGO Medical Technology Co., Ltd. In the CNAS and CMA schedules the test object is "medical device packaging materials" and the limitation field is empty; the IAS scope lists whole standards.
| Item | Standard | Clause | Notes / limitations |
|---|---|---|---|
| Seal strength | ASTM F88/F88M-23 | No clause listed | CNAS L22083; effective 2026-03-09; no limitation stated; not on the CMA schedule |
| Seal strength | YY/T 0681.2-2010 | No clause listed | CNAS L22083; effective 2026-03-09; no limitation stated |
| Seal strength | YY/T 0681.2-2010 | No clause listed | CMA 240015340087; effective 2024-11-25; no limitation stated |
| Whole standard | ASTM F88/F88M | Whole standard | IAS TL-1019; no edition year; confirm the edition with the laboratory before an IAS report against a specific edition |
| Whole standard | YY/T 0681.2 | Whole standard | IAS TL-1019; no edition year; confirm the edition with the laboratory before an IAS report against a specific edition |
Where SUNGO performs the test and under which accreditation
The test is performed in Shanghai, at the laboratory of Shanghai SUNGO Medical Technology Co., Ltd., 958 Kangqiao East Road, Pudong New Area, which issues the reports.
- CNAS accreditation, CNAS L22083. The schedule lists seal strength under ASTM F88/F88M-23 and YY/T 0681.2-2010, so reports can carry the CNAS mark. The CNAS certificate states that CNAS is a signatory to the ILAC and APAC mutual recognition arrangements.
- CMA qualification, certificate 240015340087. The schedule lists YY/T 0681.2-2010 only. The CMA mark applies only to scheduled items and the certificate states it is valid within the People's Republic of China; an ASTM F88 test cannot carry it.
- IAS accreditation, TL-1019. ASTM F88/F88M and YY/T 0681.2 are listed as whole standards without edition years; confirm the edition before an IAS report is issued.
Hefei SUNGO Medical Technology Co., Ltd. is a separate legal entity with its laboratory in Zipeng Town, Feixi County, Hefei; its scope does not include this test.
Validation of forming, sealing and assembly processes under ISO 11607-2 or GB/T 19633.2 is not within SUNGO's accreditation scope; SUNGO provides seal strength data measured under F88 or YY/T 0681.2. Whether an overseas customer or regulator accepts a given report depends on their requirements, so please confirm before ordering.
Preparing your submission
- Standard, edition and mark: ASTM F88/F88M-23 or YY/T 0681.2-2010, and CNAS, CMA or IAS, matching the scope table.
- Test conditions: technique, width and rate. Send any specification that sets them; otherwise agree them at quotation and write them into the order. If comparing with older data, send the earlier conditions.
- Package construction: materials on each side, seal type (fin, lap and so on) and seal width; mark which side is which where the webs look alike.
- Locations and results: whether to report top, side and bottom seals separately; whether you need average peel force and which algorithm, or force versus travel plots. For a conformity statement, send the document that sets the limits.
- Preconditioning: conditioning requirements, and whether samples were sterilized, aged or transport-tested; label each state separately. Aging is described on the Shelf Life Validation page.
- Number of samples: clause 7.1 asks for enough specimens to determine representative performance; set the number from the product standard or protocol and confirm it with us before ordering.
FAQ
Can an ASTM F88 report carry the CMA mark?
No. ASTM F88 is not on the Shanghai CMA schedule. It can be reported under CNAS (F88/F88M-23) or IAS (confirm the edition first). For a CMA mark, order under YY/T 0681.2-2010.
Can 15 mm results be converted to 25 mm or 1 in.?
Note 11 says strength is proportional to width under the same conditions, but Note 10 requires a documented rationale or data for any deviation. The safer approach is to test at the width the specification calls for.
Can results from Techniques A, B and C be compared?
Not directly. Clause 4.2 says each technique affects results differently, and the precision study shows different grand averages for the same material under different techniques.
Fibers came away from the paper during peeling. Is that a failure?
F88 asks you to record every mode observed but does not rule on acceptability. That depends on the product or packaging specification; if it addresses failure modes, send it with the order.
Can SUNGO perform sealing process validation?
Process validation under ISO 11607-2 and GB/T 19633.2 is not within SUNGO's accreditation scope. SUNGO can test samples you sealed at different settings under F88 or YY/T 0681.2 and report the seal strength data.
Requesting a quotation
For seal strength testing under ASTM F88/F88M or YY/T 0681.2-2010, start with the Sterile Medical Device Packaging Validation page. For how packaging validation links with sterilization validation, see Sterile Barrier Systems: Packaging and Sterilization Validation. To request a quotation, use the Contact page and send the package construction, seal type, standard and edition, the report mark needed, the technique and width required, and any preconditioning such as sterilization or aging. We will reply item by item against the CNAS, CMA and IAS scopes.
About SUNGO Lab: What We Test
SUNGO Lab is made up of two independent companies, Shanghai SUNGO Medical Technology Co., Ltd. and Hefei SUNGO Medical Technology Co., Ltd., and focuses on medical device testing. Our core service lines are:
- Wheelchair and mobility aid testing (Hefei laboratory): manual and powered wheelchairs, scooters, walking aids and crutches to the ISO 7176 series (excluding Part 19 crash testing and Part 20 standing wheelchairs), ANSI/RESNA WC-1/WC-2, EN 12183, EN 12184, the GB/T 18029 series and GB/T 12996-2024. Which accreditation (CNAS, CMA or IAS) covers each standard is as listed in our certificate scopes. See Wheelchair testing for FDA 510(k) and RESNA.
- Medical electrical safety and EMC (Hefei laboratory, IAS accredited, certificate TL-1119): IEC 60601-1, IEC 60601-1-2, IEC 60601-1-8, IEC 60601-1-11 and ISO 80601-2-69, with the corresponding Chinese standards GB 9706.1 and YY 9706.102.
- Testing for registration in China and overseas: we plan testing to the standards your target market requires (NMPA, FDA 510(k), EU CE marking and others) and issue the test reports for your submission; whether a report is accepted is decided by the regulator.
Our Shanghai laboratory also tests medical masks, gloves, surgical gowns, sterile packaging and sterilization-related items. CNAS and IAS are both signatories to the ILAC MRA. Send your product, target markets and standards through our contact page and we will confirm which laboratory and which accredited scope covers each test.